Burnishing with Steel Shot

The following guide for Steel Tumbling Media Burnishing provides some basic guidelines prior to using Steel Tumbling Media in either a Vibratory Tumbler or Barrel Tumbler.

Burnishing with Steel Tumbling Media in a Vibratory Finishing Machine

  • Vibration setting should be set at a maximum or close to maximum.
  • The Tub or Bowl should be filled 55-75% with Steel Tumbling Media and parts.
  • Use a volume ratio of three parts Steel Tumbling Media to one part of parts.
  • Use a mixture of large Steel Tumbling Media (3/16” – 50-70%) and small Steel Tumbling Media (1/8” – 30-50%). Large Steel Tumbling Media increases action.
  • A small quantity of water should be pumped into the Tub or Bowl.
  • A ratio of one ounce of Liquid Finishing Compound to each gallon of water is recommended.
  • Compounds that contain soap (usually Powder Finishing Compounds) should not be used. Instead, a Liquid Finishing Compound with a detergent component is advised.
  • Steel Tumbling Media will not Burnish if it is not polished.
  • Change compound and water every 4 hours of operating time.

Burnishing with Steel Tumbling Media in a Barrel Tumbler

  • The most effective action in a Barrel Tumbler is achieved when the Barrel Tumbler is filled to 50% of its total capacity. At this level, you will also find that your parts are less likely to damage each other. With this in mind, fill the Barrel halfway with Steel Tumbling Media and parts. Use a volume ratio of three parts Steel Tumbling Media to one part of parts (i.e. jewelry).
  • Place sufficient water in the Barrel Tumbler to cover the load (Steel Tumbling Media and parts) by 1 to 2 inches.
  • Add 1 teaspoon of Kramco 910 Burnishing Powder Finishing Compound for each quart of water. The Barrel should be rinsed out after every run. Fresh water and compound should be used for the next run.
  • Processing time for Burnishing can be from 1 to 20 hours. Soft metals will take less time than hard metals. When the object of Burnishing is to brighten recessed areas or produce a smooth surface, the run will take a minimum of 3 to 4 hours.
  • Store Steel Tumbling Media in a Barrel or plastic container. Cover Steel Tumbling Media with water and a rust-inhibiting compound, such as Kramco 510 Rust Inhibiting Powder Finishing Coumpound shing Compound.
  • Steel Tumbling Media will only Polish if it is bright and light colored.

Procedure for Cleaning Dark or Lightly Rusted Steel Tumbling Media

Rinse out barrel. Add sufficient fresh water to cover the Steel Tumbling Media by one or two inches. Add one teaspoon of Kramco 750 Cleaning Powder Finishing Coumpound to the Barrel for each gallon of water. Run for one or two hours. Repeat if Steel Tumbling Media is not bright and light colored. Rinse out after run. You can now begin normal Burnishing process.

When a project needs finishing, start here. The last stop for all your surface finishing needs.